    Microfluidics 1 - Mold Fabrication: Spin Coating of Photoresist

    Serhat S, C. Yunus Sahan

    Published: 2021-08-23 DOI: 10.17504/protocols.io.bxkjpkun
    AI 解读
    浏览 1567

    Abstract

    Microfluidic Lab-on-a-chip technology has several different materials and fabrication methods. PDMS (PolyDiMethylSiloxane) is a well-known material and due to its several advantages, it is one of the most prefered material. PDMS chip fabrication technique requires an initial master mold on which replicates can be done. Su8 is a photoresist resin used in MEMS technology for relatively thick structures. PDMS microfluidic chips fabrication is suitable for SU8+Si wafer molds. This protocol describes the coating of SU8 photoresist on silicon wafers by spin coating method in our laboratories.

    Before start

    This protocol is derived from

    [Reference: Processing guidelines for permanent epoxy negative photoresist SU8 2025, SU8 2035, SU8 2050 and SU8 2075, MicroChem company ]

    Steps

    SpinCoater Instrument Adjustment

    1.

    Dispense 1ml of photoresist (SU8) resin for each inch (25mm) of Si wafer substrate diameter.

    Spin at 500 rpm for 10 seconds with an acceleration of 100 rpm/second.

    Spin at "N" rpm for 30 seconds with an acceleration of 300 rpm/second.

    Expected results of photoresist thickness:

    40um film thickness with N=4000 rpm spin of SU8 2050

    25um film thickness with N=4000 rpm spin of SU8 2025

    75um film thickness with N=2000 rpm spin of SU8 2050

    40um film thickness with N=2000 rpm spin of SU8 2025

    Safety information
    The step is performed inside the Class 100.000 cleanroom and in a fume hood.

    Spin Coater Run

    2.

    Place the wafer in the spin coater and run the device.

    Microscope slides, Si/SiO2 wafers, and glass/PMMA wafers are alternatives substrates.

    Equipment

    ValueLabel
    Spin CoaterNAME
    LaurellBRAND
    WS-650MZ-23NPPBSKU
    www.nehirbt.com.trLINK

    Soft Baking of SU8 Coated Wafer

    3.

    Soft baking is done depending on the thickness of the coated photoresist film.

    It is a few minutes of baking at 65oC and 5-15 minutes of baking at 95oC are applied.

    Equipment

    ValueLabel
    Hot PlateNAME
    ElectromagBRAND
    LB.EM.M4060SKU
    www.nehirbt.com.trLINK

    Stocking the Coated Wafer

    4.

    In a petri plate, covered tightly with aluminum foil, photoresist-coated wafers can be stored in the cleanroom at room temperature for approximately one month.